Material: Electrolytic Tough Pitch (ETP) Copper | Document Version: 2.0 | Date: June 2025
Material Identification
Designation System | Code | Standard Reference |
---|---|---|
UNS Number | C11000 | ASTM B124/B152 |
European Standard | CW004A | EN 1412 |
Japanese Standard | C1100 | JIS H3100 |
ISO Designation | Cu-ETP | ISO 1634-1 |
Chemical Composition (wt%)
Element | Minimum | Maximum | Typical | Notes |
---|---|---|---|---|
Copper + Silver | 99.90 | — | 99.95 | Primary constituent |
Oxygen | 0.015 | 0.040 | 0.025 | 150-400 ppm as Cu₂O |
Silver | — | 0.030 | 0.015 | Counted in copper total |
Lead | — | 0.005 | 0.002 | Impurity control |
Iron | — | 0.005 | 0.002 | Impurity control |
Tin | — | 0.002 | <0.001 | Impurity control |
Zinc | — | 0.002 | <0.001 | Impurity control |
Total Other Impurities | — | 0.050 | 0.020 | Excluding oxygen |
Physical Properties at 20°C
Property | Metric Value | Imperial Value | Test Method |
---|---|---|---|
Electrical Properties | |||
Electrical Conductivity | ≥58 MS/m (100% IACS) | ≥100% IACS | ASTM E1004 |
Electrical Resistivity | 1.724 µΩ·cm | 6.79 µΩ·in | ASTM B193 |
Temperature Coefficient | 0.00393 /°C | 0.00218 /°F | — |
Thermal Properties | |||
Thermal Conductivity | 390 W/m·K | 270 BTU·ft/(h·ft²·°F) | ASTM E1461 |
Specific Heat Capacity | 0.385 J/g·K | 0.092 BTU/(lb·°F) | — |
Thermal Expansion (20-300°C) | 16.5 × 10⁻⁶ /°C | 9.2 × 10⁻⁶ /°F | ASTM E228 |
Physical Constants | |||
Density | 8.94 g/cm³ | 0.323 lb/in³ | — |
Melting Point | 1,083°C | 1,981°F | — |
Elastic Modulus | 117 GPa | 17,000 ksi | ASTM E111 |
Poisson’s Ratio | 0.34 | 0.34 | — |
Mechanical Properties
Annealed Condition (O60/O61)
Property | Value Range | Typical | Test Standard |
---|---|---|---|
Ultimate Tensile Strength | 210-250 MPa | 230 MPa | ASTM E8/E8M |
0.2% Yield Strength | 70-100 MPa | 85 MPa | ASTM E8/E8M |
Elongation (50mm gauge) | 45-55% | 50% | ASTM E8/E8M |
Rockwell Hardness | 45-65 HRB | 55 HRB | ASTM E18 |
Cold-Worked Tempers
Temper | Reduction (%) | UTS (MPa) | YS 0.2% (MPa) | Elongation (%) | Hardness (HRB) |
---|---|---|---|---|---|
H02 | ~25 | 300 | 200 | 25 | 70 |
H04 | ~50 | 350 | 280 | 10 | 85 |
H08 | ~75 | 400 | 320 | 5 | 95 |
Fatigue Properties
Test Condition | Endurance Limit | Cycles | Notes |
---|---|---|---|
Rotating Beam (R = -1) | ~90 MPa | 10⁷ | Room temperature |
Axial Load (R = 0.1) | ~120 MPa | 10⁷ | Annealed condition |
Fabrication Characteristics
Process | Suitability | Parameters/Notes |
---|---|---|
Forming Operations | ||
Cold Drawing | Excellent | Deep drawing ratio r̄ ≈ 2.0 |
Bending | Excellent | Min. bend radius = 1t (annealed) |
Stamping | Excellent | Clean blanking possible |
Hot Working | Good | Temperature range: 700-900°C |
Joining Methods | ||
Soft Soldering | Excellent | Use rosin-based flux |
Silver Brazing | Excellent | Preferred for HVAC applications |
Resistance Welding | Fair | Control expulsion |
TIG/MIG Welding | Limited | Porosity issues |
Friction Stir Welding | Good | Solid-state process |
Machining | ||
General Machinability | Good | Tool life index: 20 (Brass = 100) |
Recommended Speed | 120 m/min | Carbide tools with flood coolant |
Corrosion Resistance
Environment | Performance | Corrosion Rate | Comments |
---|---|---|---|
Atmosphere (Urban) | Excellent | <0.01 mm/year | Forms protective oxide |
Fresh Water | Excellent | <0.005 mm/year | Suitable for potable water |
Seawater (static) | Good | 0.02-0.05 mm/year | Copper-nickel preferred >2 m/s |
Neutral Soil | Good | Variable | PE sleeve in acidic conditions |
Reducing Atmospheres | Poor | — | Risk of hydrogen embrittlement |
Applications by Industry
Industry Sector | Typical Applications | Key Requirements Met |
---|---|---|
Electrical Power | Busbars, switchgear contacts, transformer windings | High conductivity, reliability |
Electronics | PCB traces, connectors, RF components | Conductivity, solderability |
HVAC/Refrigeration | Heat exchanger tubes, refrigerant lines | Thermal conductivity, corrosion resistance |
Construction | Plumbing, roofing, architectural elements | Durability, formability, aesthetics |
Automotive | Radiators, brake lines, electrical harnesses | Heat transfer, vibration resistance |
Marine | Heat exchangers, piping systems | Seawater compatibility |
Applicable Standards
Organization | Standard Number | Description |
---|---|---|
ASTM International | ||
B124 | Copper and Copper Alloy Bars and Rods | |
B152 | Copper Sheet, Strip, and Rolled Bar | |
B187 | Copper Busbar | |
B188 | Seamless Copper Tube | |
B837 | Seamless ID-Controlled Copper Tube | |
European Standards | ||
EN 13599 | Copper and Copper Alloys – Chemical Composition | |
EN 13601 | Copper Rod, Bar and Wire for Electrical Purposes | |
International Standards | ||
ISO 1634-1 | Wrought Copper – Chemical Composition | |
ISO 2009 | Copper and Copper Alloys – Cast Products | |
Japanese Standards | ||
JIS H3100 | Copper and Copper Alloy Sheets and Strips | |
JIS H3250 | Copper and Copper Alloy Seamless Pipes and Tubes |
Quality Control Testing
Test Category | Method | Frequency | Acceptance Criteria |
---|---|---|---|
Chemical Analysis | |||
Copper Content | OES/AAS | Each heat | ≥99.90% (incl. Ag) |
Oxygen Content | Inert gas fusion | Each heat | 0.015-0.040% |
Mechanical Testing | |||
Tensile Properties | ASTM E8/E8M | Per lot | Per specification |
Hardness | ASTM E18 | Per coil/bar | Per specification |
Electrical Testing | |||
Conductivity | ASTM E1004 | Per lot | ≥100% IACS |
Dimensional Control | |||
Thickness/Diameter | Micrometry | Continuous | ±tolerance |
Non-Destructive Testing | |||
Surface Quality | Eddy current | As required | No detectable defects |
Storage and Handling
Parameter | Recommendation | Rationale |
---|---|---|
Storage Environment | Dry, ventilated area | Prevent tarnishing |
Humidity Control | <60% RH | Minimize oxidation |
Temperature | Ambient | Avoid thermal cycling |
Packaging | Moisture barrier, VCI paper | Corrosion prevention |
Handling | Clean gloves, avoid scratching | Maintain surface quality |
Technical Notes
Oxygen Content Impact:
- Enhances recrystallization and grain refinement
- Provides balanced strength-ductility relationship
- Slightly reduces conductivity vs. oxygen-free copper
- Risk of hydrogen embrittlement in reducing atmospheres
Temperature Limitations:
- Softening begins around 200°C
- Creep considerations above 150°C for long-term loading
- Recrystallization temperature: 200-300°C depending on cold work
Design Considerations:
- Coefficient of thermal expansion must be considered in multi-material assemblies
- Galvanic compatibility with other metals in wet environments
- Joint design critical for high-current applications
Document prepared in accordance with: ASTM, EN, ISO, and JIS standards
For additional technical support: Contact your material supplier or accredited testing laboratory